EN 10216 EU standards
Date: 2022-01-07
EN 10216: EU standards
EN 10216-1: EU standards
EN 10216-2: EU standards
Purpose:
For the boiler pipes, tobacco pipes, super heater tubes, air pre-heater tubes.
Following consultations, can also be supply other grades of steel pipe.
Mechanical properties:
Chemical composition:
Post time: Jun-07-2022
Standard
Grade
Tensile strength (MPa)
Yield strength (MPa)
Elongation (%)
EN10216-1
P195
320~440
≥195
≥27
EN10216-1
P235
360~500
≥235
≥25
EN10216-1
P265
410~570
≥265
≥23
EN10216-2
P195GH
320~440
≥195
≥27
EN10216-2
P235GH
360~500
≥235
≥25
EN10216-2
P265GH
410~570
≥265
≥23
EN10216-2
13CrMo4-5
440~590
≥290
≥22
EN10216-2
10CrMo9-10
480~630
≥280
≥22
Standard
Grade
Chemical Composition
Chemical Composition
Chemical Composition
Chemical Composition
Chemical Composition
Chemical Composition
Chemical Composition
Chemical Composition
Chemical Composition
Chemical Composition
Standard
Grade
C
Si
Mn
P
S
Cr
Mo
Cu
Ni
V
EN10216-1
P195
≤0.13
≤0.35
≤0.70
≤0.025
≤0.020
≤0.30
≤0.06
≤0.30
≤0.30
/
EN10216-1
P235
≤0.16
≤0.35
≤1.20
≤0.025
≤0.020
≤0.30
≤0.06
≤0.30
≤0.30
/
EN10216-1
P265
≤0.20
≤0.40
≤1.40
≤0.025
≤0.020
≤0.30
≤0.06
≤0.30
≤0.30
/
EN10216-2
P195GH
≤0.13
≤0.35
≤0.70
≤0.025
≤0.020
≤0.30
≤0.06
≤0.30
≤0.30
/
EN10216-2
P235GH
≤0.16
≤0.35
≤1.20
≤0.025
≤0.020
≤0.30
≤0.06
≤0.30
≤0.30
/
EN10216-2
P265GH
≤0.20
≤0.40
≤1.40
≤0.025
≤0.020
≤0.30
≤0.06
≤0.30
≤0.30
/
EN10216-2
13CrMo4-5
0.10~0.17
≤0.35
0.40~0.70
≤0.025
≤0.020
0.70~1.15
0.40~0.60
≤0.30
≤0.30
/
EN10216-2
10CrMo9-10
0.08~0.14
≤0.50
0.30~0.70
≤0.025
≤0.020
2.00~2.50
0.90~1.10
≤0.30
≤0.30
/